PA6 BKV 240 H2.0 XCP 901510德國朗盛Durethan 40%玻纖增強耐沖擊熱老化穩定尼龍6塑料(18024445500)
PA 6, 40 % glass fibers, injection molding, improved impact strenght, heat-aging stabilized
ISO Shortname: ISO 1874-PA 6-HI,GHR,14-110,GF40
Property Test Condition Unit Standard guide value
d.a.m. cond.
Rheological properties
C Molding shrinkage, parallel 60x60x2; 280 °C / MT 80 °C; 600 bar % ISO 294-4 0.25
C Molding shrinkage, transverse 60x60x2; 280 °C / MT 80 °C; 600 bar % ISO 294-4 0.73
Post- shrinkage, parallel 60x60x2; 120 °C; 4 h % ISO 294-4 0.03
Post- shrinkage, transverse 60x60x2; 120 °C; 4 h % ISO 294-4 0.13
Mechanical properties (23 °C/50 % r. h.)
C Tensile modulus 1 mm/min MPa ISO 527-1,-2 11000 6000
C Nominal strain at break 50 mm/min % ISO 527-1,-2 10
C Tensile Stress at break 5 mm/min MPa ISO 527-1,-2 160 100
C Tensile Strain at break 5 mm/min % ISO 527-1,-2 5.5 11
C Charpy impact strength 23 °C kJ/m² ISO 179-1eU 110 125
C Charpy impact strength -30 °C kJ/m² ISO 179-1eU 105
C Charpy notched impact strength 23 °C kJ/m² ISO 179-1eA 28 40
C Charpy notched impact strength -30 °C kJ/m² ISO 179-1eA 17
Izod impact strength 23 °C kJ/m² ISO 180-1U 95 110
Izod impact strength -30 °C kJ/m² ISO 180-1U 95
Izod notched impact strength 23 °C kJ/m² ISO 180-1A 28 40
Izod notched impact strength -30 °C kJ/m² ISO 180-1A 17
Flexural modulus 2 mm/min MPa ISO 178-A 10100 6300
Flexural strength 2 mm/min MPa ISO 178-A 255 150
Flexural strain at flexural strength 2 mm/min % ISO 178-A 5 5.5
Flexural stress at 3.5 % strain 2 mm/min MPa ISO 178-A 235 125 |